DuPont de Nemours, Inc. · NYSE:DD

DuPont de Nemours — DuPont — Technical Presentation (April 2006)

42 slides from DuPont de Nemours's technical presentation, Apr 4, 2006

  1. Slide 1: DuPont ETPV Web Seminar

    DuPont™ ETPV Web Seminar THE THERMOPLASTIC RUBBER THAT RESISTS OIL AND HEAT April 4, 2006

  2. Slide 2: DuPont ETPV Web Seminar - Sponsored by

    2 DuPont™ ETPV Web Seminar Sponsored by: Mark Jacobson DuPont™ ETPV Business Manager 4/11/2008

  3. Slide 3: DuPont ETPV Web Seminar

    DuPont™ ETPV Web Seminar THE THERMOPLASTIC RUBBER THAT RESISTS OIL AND HEAT The information and suggestions provided in this on-line seminar are based on data believed to be reliable, but the DuPont Company makes no warranties express or implied as to their accuracy and assumes no responsibility or

  4. Slide 4: DuPont ETPV Web Seminar

    DuPont™ ETPV Web Seminar THE THERMOPLASTIC RUBBER THAT RESISTS OIL AND HEAT The information and suggestions provided in this on-line seminar are based on data believed to be reliable, but the DuPont Company makes no warranties express or implied as to their accuracy and assumes no responsibility or

  5. Slide 5: Presented by

    5 DuPont™ ETPV Web Seminar Presented by: Dan Saunders North America Processing Specialist Coreen Y. Lee Development Specialist, Flexible Solutions Group 4/11/2008

  6. Slide 6: Agenda

    6 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 7 Summary 4/11/2008

  7. Slide 7: Why are you interested in DuPont ETPV?

    7 Why are you interested in DuPont™ ETPV? Because replacing cross-linked rubber with a thermoplastic material will significantly reduce costs. 4/11/2008

  8. Slide 8: Why DuPont ETPV versus Thermoset Rubber

    8 Why DuPont™ ETPV versus Thermoset Rubber 4/11/2008

  9. Slide 9: Why DuPont ETPV versus Thermoset Rubber

    9 Why DuPont™ ETPV versus Thermoset Rubber Silicone Rubber DuPont™ ETPV Savings No of cavities 4 4 Annual volume 1000000 1000000 Cost per machine hour 24 30 Density 1.15 1.08 g/cm 2 Material price 10.80 11.52 USD/kg Part net weight 10.0 9.4 grams Waste 10.0 1.0 % Part weight including waste 11.0 9.5

  10. Slide 10: DuPont ETPV engineering thermoplastic vulcanizates

    10 DuPont™ ETPV engineering thermoplastic vulcanizates The thermoplastic rubber that resists oil and heat a high performance cross-linked elastomer dispersed in a high performance thermoplastic elastomer ! Recycling code (ISO 11469) > AEM + TPC - ET < ! AEM = ethylene acrylic elastomer ! TPC - ET =

  11. Slide 11: DuPont ETPV and cross-linked rubbers heat resistance

    11 DuPont™ ETPV and cross-linked rubbers 300 Kalrez® 275 250 Viton® 225 Silicone Heat resistance, °C 200 Fluorosilicone Vamac® 175 DuPont™ ETPV EPDM Polyacrylate (ACM ) HNBR 150 EVA Hypalon® (high VA) Epichlorohydrine (ECO) PU 125 Ethylene-propylene Neoprene Butyl Nitrile (NBR) 100 75 SBR & NR 50 No

  12. Slide 12: Agenda

    12 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 7 Summary 4/11/2008

  13. Slide 13: Product Line

    13 Product Line Standard grades 60A01L NC010 60 Shore A, lubricated 70A01 NC010 70 Shore A 80A01 NC010 80 Shore A 90A01 NC010 90 Shore A 95A02 NC010 95 Shore A for blow molding or extrusion Heat stabilized grades 60A01HSL BK001 60 Shore A, lubricated 90A01HS BK001 90 Shore A 95A02HS BK001 95 Shore A

  14. Slide 14: Elongation at break retention, air oven aging

    14 Elongation@break - 50% Retention for DuPont™ ETPV Air Oven Aging 100000 10000 60AHS Time (h) 60A 90AHS 90A 1000 100 120 130 140 150 160 170 180 Temperature (°C) 4/11/2008

  15. Slide 15: DuPont ETPV Dexron VI 150°C Aging

    15 DuPont™ ETPV - Dexron VI @150°C Aging 200 180 %Retained - Stress@break 160 140 120 100 80 60 40 DuPont™ ETPV - Dexron VI @150°C Aging 20 140 0 120 0 500 1000 1500 2000 2500 3000 3500 %Retention - Strain@break Time (h) 100 80 60 ETPV 60A01 HSL ETPV 60A01L 40 ETPV 90A01 HS 20 0 0 500 1000 1500 2000

  16. Slide 16: DuPont ETPV Dexron VI 150°C Aging

    16 DuPont™ ETPV - Dexron VI @150°C Aging 90.0 80.0 70.0 Shore A Hardness 60.0 50.0 DuPont™ ETPV - Dexron VI @150°C Aging 40.0 20.0 30.0 15.0 20.0 0 500 1000 1500 2000 2500 Time(h) Volume Change 10.0 5.0 ETPV 60A01 HSL ETPV 60A01L ETPV 90A01 HS 0.0 -5.0 0 500 1000 1500 2000 2500 3000 3500 Time (h) 4/

  17. Slide 17: Agenda

    17 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 7 Summary 4/11/2008

  18. Slide 18: Agenda

    18 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 7 Summary 4/11/2008

  19. Slide 19: Part Design—Flexural Seals

    19 Part Design—Flexural Seals Strain (%) -58% +13% 0% -10% Mix of compression and tensile strain. Mainly compression strain. Highest Highest stress are located on small stress located on nearly all part areas (in the skin of the lip) DuPont™ DuPont™ ACM 60 Shore A ETPV60A01 ETPV90A01 Compression set

  20. Slide 20: Part Design—Adhesion

    20 Part Design—Adhesion Design parts with mechanical locks supplemented by chemical adhesion Adhesive failure Cohesive failure DuPontTM ETPV *ISO 527-1 (1A tensile properties) 4/11/2008

  21. Slide 21: Agenda

    21 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 7 Summary 4/11/2008

  22. Slide 22: Agenda

    22 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 7 Summary 4/11/2008

  23. Slide 23: Tool Design—Ejection

    23 Tool Design—Ejection Automatic ejection in a tool designed Parts may stick in the tool if it is not for soft materials designed/modified for DuPont™ ETPV 4/11/2008

  24. Slide 24: Tool Design—Ejection

    24 Tool Design—Ejection Sprue Design—Hot sprue and runner if possible, otherwise: ! Taper 3° to 5° ! Short ! Semi-Polished ! Semi-Permanent Surface Treatment* Tool Draft ! Ample 1° to 2° Tool Surface ! Textured or Matte Surface (24 Charmilles) ! Semi-Permanent Surface Treatment* Ejectors ! Air aided

  25. Slide 25: Tool Design—Mold shrinkage

    25 Tool Design—Mold shrinkage Shrinkage influenced by: Material grade Molding conditions Part geometry Grade X Flow I Flow 60A01 1.4% 4.7% 80A01 1.2% 2.3% 90A01 1.4% 1.5% *ISO 294-4 60x60x2 mm plaques at recommended molding conditions 4/11/2008

  26. Slide 26: Agenda

    26 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 7 Summary 4/11/2008

  27. Slide 27: Processing

    27 Processing Dry Material Max recommended moisture content for processing: < 0.08% Desiccant dryer; 2–4 hours at 80°C (175°F) Purge Press With low or high density PE Five Stages of the Molding Cycle Heat Flow Form Cool Eject 4/11/2008

  28. Slide 28: Processing—Heat/Melt the Plastic

    28 Processing—Heat/Melt the Plastic High viscosity and shear Can use GP screw Verify ability to maintain barrel set points Low backpressure: 1–2 MPa (<300 ppsi) Measure plastic (melt) temperature Grade Melt T °C (°F) 60A, 70A 250–260 (480–500) 80A, 90A 240–250 (465–480) 4/11/2008

  29. Slide 29: Processing—Flow/Move the Plastic

    29 Processing—Flow/Move the Plastic Fill part 99% full using speed control Transfer on position Slow speed 15–50 mm/s (0.6–2.0˝/s) Melt being injected Flow length of DuPont™ ETPV 90A01 NC010 60A01LNC010 4/11/2008

  30. Slide 30: Processing—Form/Pack and Hold

    30 Processing—Form/Pack and Hold Decreasing pressure profile 60–25 MPa (8700–3600 ppsi) 6 s hold time per 1 mm wall thickness Filling Room Door Corridor Packing and Holding Crystallization order Put more material in to avoid internal voids. Door and corridor have to be kept open. 4/11/2008

  31. Slide 31: Runner and Gate Recommendations

    31 Processing - Form/Pack and Hold - Runner and Gate Recommendations Hot runner is preferred Cold runner is acceptable Gate stays open longer Fan, diaphragm or “crystalline” design No demolding sprue Tunnel “Crystalline” Design No specific issues with • thermal stability • wear due to filler T = the

  32. Slide 32: Processing—Cool and Eject

    32 Processing—Cool and Eject Mold temperature 30–60°C (86–140°F) Run higher temperatures for parts requiring good dimensional stability (higher temperatures result in better crystallinity) Lower temperatures result in faster set up for ejection Part out of the mold looks good Exposure to time and te

  33. Slide 33: Processing Summary—5 Step Injection Molding Process

    33 Processing Summary—5 Step Injection Molding Process 0—DRY MATERIAL Max recommended moisture content for processing: < 0.08% Desiccant dryer; 2–4 hours at 80°C (175°F) 1—HEAT Grade Melt T °C (°F) High viscosity and shear Low backpressure: 1–2 MPa (<300 ppsi) 60A, 70A 250–260 (480–500) Measure plas

  34. Slide 34: Processing—Troubleshooting

    34 Processing—Troubleshooting Problem Suggested Solution Bridging in feed throat Reduce temp of rear zone Short shots Increase injection stroke, time, pressure If machine is at max injection pressure, increase barrel temperature Check nozzle, sprue, runner & gates for frozen material / flow restrict

  35. Slide 35: Agenda

    35 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 7 Summary 4/11/2008

  36. Slide 36: Current Applications

    36 Current Applications DuPont™ ETPV can be processed by standard thermoplastic processing techniques including: Injection molding 2K Injection molding Extrusion Blow molding 4/11/2008

  37. Slide 37: Agenda

    37 Agenda 1 Why DuPont™ ETPV 2 Product Line Portfolio and Key Properties 3 Part Design Considerations 4 Tool Design Considerations 5 Processing Considerations 6 DuPont™ ETPV Applications 6 7 Summary 4/11/2008

  38. Slide 38: Summary

    38 Summary DuPontTM ETPV offers significant opportunities for part cost reduction in high performance applications. Critical factors for success include: • Material Selection • Part Design • Tool Design • Process Optimization Maximize opportunity for program success… engage your DuPont representativ

  39. Slide 39: Summary

    39 Summary DuPontTM ETPV offers significant opportunities for part cost reduction in high performance applications. Critical factors for success include: • Material Selection • Part Design • Tool Design • Process Optimization Maximize opportunity for program success… engage your DuPont representativ

  40. Slide 40: Thank you for joining us today

    40 Thank you for joining us today. Please send in any questions using the Q&A function. We will be answering questions for the rest of the hour. Depending on demand, we may not be able to answer your question straight away. All questions will be logged and any questions unanswered at the end of the

  41. Slide 41: Copyright 2006 DuPont trademarks

    Copyright © 2006 DuPont or its affiliates. All rights reserved. The DuPont Oval Logo, DuPont™, The miracles of science™, Kalrez®, Viton®, Vamac®, Hypalon®, Hytrel®, Crastin®, Rynite®, Thermx®, Zytel®, and Delrin® are registered trademarks or trademarks of DuPont or its affiliates.

  42. Slide 42: The miracles of science