  1. Slide 1: Application Data for Submerged Arc Welding Fluxes

    APPLICATION DATA FOR SUBMERGED ARC WELDING FLUXES

  2. Slide 2: Index

    INDEX Classifica on of Submerged Arc Welding Flux... 03 Welding Parameters for Tandem Welding... 20 Automelt A82 Flux... 04 Common customer complaints on Automelt B71 Flux... 21 Automelt A82 Flux (Tube to Plate Joining – Heat Exchanger)... 05 Automelt B22 Plus Flux... 22 Automelt A82 Flux... 06 Commo

  3. Slide 3: Classification of Submerged Arc Welding Flux

    Classifica on of Submerged Arc Welding Flux Flux Classifica on Based on Descrip on 1. Agglomerated (ADOR WELDING LTD Raw materials/ Minerals mixed with silicate & a er manufacturing Agglomerated type flux only) forming required sieve size flux was baked at 700 - 1000 ⁰C. Flux Manufacturing Method 2. Fus

  4. Slide 4: Automelt A82 Flux

    Automelt A82 Flux Plate Thickness 04 – 24 mm Plate Grade SA 516 Gr 60/70, IS 2062, C-Mn Steel Type of Joint Fillet, H Beam Both side Welding Welding Posi on 2F Welding Wire Used EM12K – 1.60mm, Twin Wire Used Current Used 500 to 800 A Voltage Used 26 to 32 V Travel Speed 1100 to 1800 mm/Min Preheat

  5. Slide 5: Automelt A82 Flux (Tube to Plate Joining – Heat Exchanger)

    Automelt A82 Flux (Tube to Plate Joining – Heat Exchanger) Plate Thickness & Grade 06 mm - IS 2062 Pipe Dimension & Grade 63 mm OD & 4 mm Thickness – SA 210 Gr A1 Type of Joint Fillet Welding Posi on 2F Welding Wire Used EM12K – 1.60mm, Single Wire Used Current Used 350 A Voltage Used 25 V Note: If

  6. Slide 6: Automelt A82 Flux

    Automelt A82 Flux As per AWS D1.1 Table 5.8 Minimum fillet weld size & welding Parameters to achieve the weld size Base Plate Fillet Size, Sl No Travel speed Sr. No. Wire Dia, mm Current (Amp) Voltage (V) Thickness mm (mm/Min) 1 Up to 6 mm 3 400 - 550 26 - 28 1600 - 1800 2 6 to 12 5 1.6 mm - Twin 500

  7. Slide 7: Common customer assistance on Automelt A82 Flux

    Common customer assistance on Automelt A82 Flux Problem Reason for the Problem Solu on to the Problem Porosity on weld centreline 1. Excess voltage leads to lack of fusion 1. Reduce the voltage Point by Point. and it is reason for Porosity Less voltage leads to Convex bead & 2. Posi on of Welding Wi

  8. Slide 8: Automelt A81

    Automelt A81 Plate Thickness 8 – 20 mm Plate Grade IS 2062 Type of Joint Fillet Welding Posi on 2F Welding Wire Used EM12K – 1.6 mm, Twin Wire Used Current Used 530 A Voltage Used 28 – 29 V Travel Speed 1200 mm/Min Preheat NA (Ambient Temperature: 30-40º Celsius) Inter-pass Temperature NA Single or

  9. Slide 9: Common customer assistance on Automelt A81 Flux

    Common customer assistance on Automelt A81 Flux Problem Reason for the Problem Solu on to the Problem Porosity on weld centreline 1. Excess voltage leads to lack of fusion 1. Reduce the voltage Point by Point. and it is reason for Porosity Less voltage leads to Convex bead & 2. Posi on of Welding Wi

  10. Slide 10: Automelt A55 (SPL) Flux

    Automelt A55 (SPL) Flux Plate Thickness 10 – 30 mm Plate Grade SA516 Gr 60 To SA 516 Gr 60 / SA 516 Gr 60 to SA 836 class 1 Type of Joint Groove - Single V Joint Design Ceramic Backing, Root Gap 1 -2 mm, Root Face 2-3 mm Welding Posi on 1G Welding Wire Used EL8 – 3.15 mm, Single Wire Used Current Us

  11. Slide 11: Common customer assistance on Automelt A55 Spl Flux

    Common customer assistance on Automelt A55 Spl Flux Problem Reason for the Problem Solu on to the Problem Slag S cky on Root Run 1. Higher Voltage 1. Reduce the voltage point by point 2. Lower Travel speed 2. Increase the travel speed slightly 3. Fine Flux 3. Coarse Flux was suitable Weld Joint Cros

  12. Slide 12: Automelt A57

    Automelt A57 Plate Thickness 12 mm – Pipe Longitudinal weld Plate Grade C-Mn Steel Type of Joint Groove - Double V Welding Posi on 1G Welding Wire Used EL8 – 3.15 mm, Single Wire Used Current Used 400 to 500 A Voltage Used 38 to 40 V Travel Speed 300 to 340 mm/Min Preheat NA (Ambient Temperature: 30

  13. Slide 13: Automelt A57 - Cylinder Manufacturing

    Automelt A57 - Cylinder Manufacturing Plate Thickness 3 mm Plate Grade C-Mn Steel Type of Joint Bu Joint Type Joint Design 3mm + 3mm = 6mm Bead on Plate Welding Wire Used EL8 – 2.50 mm, Single Wire Used Current Used 450 A Voltage Used 27 - 28V Travel Speed 1200 mm/Min Preheat NA (Ambient Temperature

  14. Slide 14: Common customer assistance on Automelt A57 Flux

    Common customer assistance on Automelt A57 Flux Problem Reason for the Problem Solu on to the Problem Pock Marks 1. Rusty base plates 1. Remove the rust from base plates 2. Moisture in flux 2. Redry flux at 300º Celsius for 2 Hr Porosity 1. Excess Voltage 1. Reduce the voltage point by point Moisture

  15. Slide 15: Automelt B31 / Grade 1V Flux

    Automelt B31 / Grade 1V Flux Plate Thickness 18 - 36 mm Plate Grade C –Mn Steel Type of Joint Fillet Joint & Lab Joint Welding Posi on 1F Welding Wire Used EL8 / Grade A (W1) – 4.00 mm, Single Wire Used Current Used 600 – 625 A Voltage Used 27 to 29 V Travel Speed 300 - 320 mm/Min Preheat NA (Ambien

  16. Slide 16: Common customer assistance on Automelt B31 / Grade IV

    Common customer assistance on Automelt B31 / Grade IV Problem Reason for the Problem Solu on to the Problem Porosity on root run 1. Excess voltage will not melt the fillet 1. Reduce the voltage.Recommended weld root. Voltage was 28 – 30 V 2. Slow Travel speed will make the 2. Increase the Travel spee

  17. Slide 17: Automelt B71 Flux

    Automelt B71 Flux Plate Thickness 12 - 72 mm Plate Grade IS 2062 Type of Joint Groove Joint Design Single / Double V bu joint, Root gap-0 to 3mm, Root face: 04 mm, Included angle 60⁰ Welding Posi on 1G Welding Wire Used EM12K – 4.00 mm, Single Wire Used Current Used 320 - 360 A for root run & 450 to

  18. Slide 18: Automelt B71 Flux (Fillet 2F Application)

    Automelt B71 Flux (Fillet 2F Applica on) Plate Thickness 16, 40, 50 mm Plate Grade IS 2062 Type of Joint Fillet Welding Posi on 2F Welding Wire Used EM12K – 3.15 mm, Single Wire Used Current Used 480 A Voltage Used 29 V Travel Speed 500 – 550 mm/min for root run & 300 mm/min for subsequent passes Pr

  19. Slide 19: Automelt B71 Flux (Tandem Application)

    Automelt B71 Flux (Tandem Applica on) Plate Thickness 10 – 100 mm Plate Grade SA 515 Gr 70 Type of Joint Groove - Longitudinal Pipe Joint Design Single V - 60⁰ Bevel Welding Posi on 1G Welding Wire Used EM12K – 4.00 mm, Tandem Wire. Preheat NA (Ambient Temperature: 30⁰ Celsius) Inter-pass Temperatur

  20. Slide 20: Welding Parameters for Tandem Welding

    Welding Parameters for Tandem Welding Root Run Subsequent Passes nd DC power Source AC Power Source DC power Source AC Power Source 2 AC Power Source EL8 Wire - 4.00 mm EL8 Wire - 4.00 mm EL8 Wire - 4.00 mm EL8 Wire - 4.00 mm EL8 Wire - 4.00 mm Current (A) 450 425 700 700 700 Voltage (V) 28 32 32 34

  21. Slide 21: Common customer assistance on Automelt B71 Flux

    Common customer assistance on Automelt B71 Flux Problem Reason for the Problem Solu on to the Problem Gas Marks & Pock Marks 1. Rusty Base Plate 1. Remove the rust by grinding 2. Moisture in flux 2. Redry the flux at 300º Celsius for 2 Hours Slag Removal in root run 1. Excess Voltage & slow travel spe

  22. Slide 22: Automelt B22 Plus Flux

    Automelt B22 Plus Flux Plate Thickness 45 mm Plate Grade SA 516 Gr 60/70 Type of Joint Fillet Joint Design Single V bu joint, Included angle 60⁰ Celsius Welding Posi on 1F Welding Wire Used EM12K – 4.00 mm, Single Wire Used Current Used 450 – 600 A Voltage Used 28 to 32 V Travel Speed 250 - 400 mm/M

  23. Slide 23: Common customer assistance on Automelt B22 Plus Flux

    Common customer assistance on Automelt B22 Plus Flux Problem Reason for the Problem Solu on to the Problem Gas Marks & Pock Marks 1. Rusty Base Plate 1. Remove the rust by grinding 2. Moisture in flux 2. Redry the flux at 300º Celsius for 2 Hours Welding Posi ons used in Submerged Arc Welding G - Groo

  24. Slide 24: Automelt B20 Plus Flux

    Automelt B20 Plus Flux Plate Thickness 40 mm Plate Grade C –Mn Steel Type of Joint Groove Joint Design Single V bu joint, Included angle 60⁰ Celsius Welding Posi on 1G Welding Wire Used EM12K – 4.00 mm, Single Wire Used Current Used 520 to 580 A Voltage Used 28 to 30 V Travel Speed 190 – 280 mm/Min

  25. Slide 25: Common customer assistance on Automelt B20 Flux

    Common customer assistance on Automelt B20 Flux Problem Reason for the Problem Solu on to the Problem Porosity & Flux Boiling Higher Voltage 1. Reduce the voltage & use maximum of 36 Voltage in groove Gas Marks & Pock Marks 1. Rusty Base Plate 1. Remove the rust by grinding 2. Moisture in flux 2. Red

  26. Slide 26: Automelt B41 Flux

    Automelt B41 Flux Plate Thickness 58 - 60 mm Plate Grade SA 516 Gr 60/70 Type of Joint Groove Joint Design Double V - 45⁰ Angle - SMAW Root run Welding Posi on 1G Welding Wire Used EH14 – 3.15 mm, Single Wire Used Current Used 400 - 550A Voltage Used 27 to 30 V Travel Speed 400 – 600 mm/Min Preheat

  27. Slide 27: Automelt B41 Flux (2G Application)

    Automelt B41 Flux (2G Applica on) Plate Thickness 58 - 60 mm Plate Grade SA 516 Gr 60/70 Type of Joint Groove Joint Design Double V - 45⁰ Angle - SMAW Root run Welding Posi on 2G Welding Wire Used EH14 – 2.5 mm, Single Wire Used Current Used 350 - 400A Voltage Used 23 to 25 V Travel Speed 360 - 370

  28. Slide 28: Common customer assistance on Automelt B41 Flux

    Common customer assistance on Automelt B41 Flux Problem Reason for the Problem Solu on to the Problem Porosity & Flux Boiling Higher Voltage 1. Reduce the voltage & use maximum of 36 Voltage in groove Gas Marks & Pock Marks 1. Rusty Base Plate 1. Remove the rust by grinding 2. Moisture in flux 2. Red

  29. Slide 29: Process variables: Effect of welding current

    Process variables Ÿ Current Ÿ Voltage Ÿ Travel speed Ÿ Polarity Effect of welding Current Higher current leads to higher penetra on & Dilu on 29 www.adorwelding.com

  30. Slide 30: Effect of welding voltage

    Effect of welding Voltage Higher Voltage increases the weld bead width & Flux consump on High welding voltage leads to lack of fusion in root run welding of groove & fillet 30 www.adorwelding.com

  31. Slide 31: Effect of travel speed and polarity

    Effect of Travel speed Weld bead width was directly propor onal to travel speed Effect of polarity Metal Flux Welding S ck out Reinforcement Depth of Wire feed deposi on consump on Welding Current Voltage speed distance Width rate polarity (A) (V) Height (mm) penetra on rate rate (mm/Min) (mm) (mm) (m

  32. Slide 32: Flux Selection Guide

    Flux Selec on Guide Ÿ SAW Flux & Wire selec on for the par cular applica on is depend on Applica on type & Mechanical requirements of the joint. (ADOR representa ve should collect both these details) Ÿ Applica on details are type & Thickness of base material to be weld, Joint design, welding speed &

  33. Slide 33: Flux Selection Guide

    Flux Selec on Guide Plate Thickness Welding Parameters Applica on Welding Machine Type Welding Consumables AWS Classifica on (mm) (Travel Speed) Automelt A82 + 4 - 24 800 - 1800 mm/min Single Wire / Twin Wire Automelt EM12K F7AZ-EM12K (1.6mm) Automelt A81 + Structural Fabrica on 6 - 24 400 - 1200 mm/

  34. Slide 34: Flux Selection Guide

    Flux Selec on Guide Plate Thickness Welding Parameters Applica on Welding Machine Type Welding Consumables AWS Classifica on (mm) (Travel Speed) Automelt B71 + 10 - 30 400 - 600 mm/min Single Wire / Twin Wire F7A4-EM12K General Fabrica on / Automelt EM12K Pressure vessels / Heavy Equipment fabrica on

  35. Slide 35: SAW Flux application - Enquiry Form

    SAW Flux applica on - Enquiry Form Ÿ Plate Thickness : Ÿ Plate Grade : Ÿ Type of Joint : Ÿ Joint Design : Ÿ Welding Posi on : Ÿ Welding Wire Used : Ÿ Current Used : Ÿ Voltage Used : Ÿ Travel Speed : Ÿ Preheat : Ÿ Inter-pass Temperature : Ÿ Single or Mul -pass : Ÿ Flux Specifica on : Ÿ Weld metal Chem

  36. Slide 36: Thank You!

    s¢ador peace of mind Thank You!

Ador Welding — Technical Presentation (March 2023) on 6ix